Introduction: Why Surface Treatment of Die-Casting Mold Base Plates Matters
Die-casting mold base plates are often treated as secondary components. They do not form the casting cavity, they do not usually contact molten metal, and they are rarely the first parts mentioned when a mold is designed. In practice, however, the base plates carry the mold, locate the cavity inserts, guide the ejector system, support slides, and absorb repeated clamping loads. A rusted water line, a galled guide pin bore, or a worn ejector plate can stop production just as effectively as a damaged cavity insert.
A typical die-casting mold base consists of an A-plate, a B-plate, ejector plates, support plates, guide pins and bushings, leader pins, wear plates, gibs, and support pillars. Common base materials include S50C or 1050 carbon steel, P20 or 1.2311 pre-hardened steel, 4140 alloy steel, and sometimes H13 for highly loaded or heat-exposed details. These materials behave differently during surface treatment, and the treatment must be matched to the material as well as to the function of the plate.
Unlike cavity inserts, base plates seldom suffer direct thermal fatigue from molten metal. Their surface treatment priorities are different. The first priority is corrosion protection, especially in water-cooling channels, pockets, and exterior faces exposed to humidity, release sprays, and washing. The second is wear and galling resistance on guide components, ejector guide holes, clamping faces, and sliding surfaces. The third is dimensional stability. A treatment that adds an uncontrolled layer to a precision bore or changes the flatness of a large plate can create more problems than it solves.
This is why surface treatment of die-casting mold base plates should be specified as a functional engineering requirement, not as a cosmetic finish. The correct treatment depends on the base material, the working environment, the expected production life, the storage and shipping conditions, and the tolerance of the features being treated.
What Makes Base Plates Different from Cavity Inserts
Cavity inserts in die casting are exposed to molten metal, high thermal gradients, erosion, soldering, and thermal fatigue. Their coatings and treatments are often selected for heat resistance, thermal shock resistance, and resistance to aluminum or zinc adhesion. Base plates operate under different conditions. They are large, structural, and usually machined to fine tolerances. They may contain deep water lines, threaded holes, dowel holes, guide pin bores, ejector guide holes, and clamping slots.
The main degradation mechanisms for base plates are:
- Rust and corrosion inside cooling channels and on exterior surfaces.
- Galling or adhesive wear on guide pins, bushings, ejector guides, and sliding wear plates.
- Brinelling, fretting, and local wear under high clamping loads.
- Dimensional drift caused by poor stress relief or by coatings applied after final machining.
- Handling damage and cosmetic deterioration during storage and shipment.
Because base plates are large, some high-end treatments are impractical for the entire plate. For example, PVD and DLC coatings are usually applied in vacuum chambers with limited size. They are common on bolted-on wear plates, gibs, ejector guide bushings, and small sliding components, but they are rarely applied to a complete A-plate or B-plate. Similarly, hard chrome is often applied selectively to wear surfaces rather than to the whole base.
A good specification therefore distinguishes between the treatment of the plate body, the treatment of internal water lines, and the treatment of separate wear or guide components.
The Main Treatment Families at a Glance
Surface treatments for die-casting mold base plates can be grouped into three families.
The first family is corrosion and rust prevention. This includes black oxide, phosphate coating, electroless nickel plating, hard chrome plating, zinc plating, and protective paint. These treatments are used on exterior faces, water lines, pockets, and non-critical surfaces.
The second family is wear and galling resistance. This includes gas nitriding, plasma nitriding, nitrocarburizing, QPQ, hard chrome, PVD coatings such as TiN and CrN, DLC, and self-lubricating electroless nickel with PTFE. These treatments are used where sliding, clamping, or repeated contact occurs.
The third family is surface conditioning and stress management. This includes shot peening, glass bead blasting, stress relief, and final grinding. These processes do not always form a protective layer, but they influence fatigue resistance, surface finish, dimensional accuracy, and coating adhesion.
In practice, these families overlap. QPQ, for example, provides both wear resistance and corrosion resistance. Electroless nickel can provide corrosion protection and, after heat treatment, useful wear resistance. Hard chrome can protect against both abrasion and moisture. The selection process is therefore about matching a treatment to the dominant failure mode of each area, not about choosing one universal finish for the entire mold base.
Corrosion and Rust Prevention Treatments
Black Oxide and Blackening
Black oxide, also called blackening or black plating, is the most common low-cost treatment for mold base plates. It is a chemical conversion process that forms a thin magnetite layer on the steel surface. The layer is usually only about 1 to 3 micrometres thick, although some suppliers quote a broader range depending on the process and the surface condition. Because the coating is a conversion layer rather than a heavy deposit, it has virtually no dimensional impact.
Black oxide is popular because it is inexpensive, improves the appearance of the plate, reduces glare in the workshop, and holds rust-preventive oil well. It is often used on exterior plate faces, clamping plates, and general machined surfaces. For a mold that will be used quickly in a dry shop, ground and black-oxided plates are often sufficient.
Black oxide has important limitations. It is not a long-term corrosion barrier, and it is not suitable for aggressive cooling water. If the water lines are left unprotected, rust can develop inside the channels even if the exterior looks black and clean. Black oxide also offers little wear resistance. It should be specified with a suitable rust-preventive oil or wax, and it should not be expected to survive long sea shipment or prolonged storage in a humid warehouse without additional protection.
Phosphate Coating
Phosphate coating, sometimes called Parkerizing, is another conversion treatment. It produces a crystalline phosphate layer on the steel surface. Manganese phosphate and zinc phosphate are both used. Typical coating thickness is in the range of a few micrometres to about ten micrometres, depending on the process and the required oil retention.
Phosphate is valued for its oil retention. The porous crystalline structure holds rust-preventive oil or wax better than a bare or black-oxided surface, which makes it useful for storage and sea shipment. It is often applied after machining and before packing. It is not a wear coating, and it should not be used as a substitute for nitriding or hard chrome on sliding surfaces.
The process sequence must be controlled. If a phosphate coating is applied before final grinding, the grinding operation will remove the coating from critical surfaces. If the phosphate is intended as a final finish, it should be applied after final machining, and any precision surfaces that must remain uncoated should be masked. Phosphate is also less attractive than black oxide for some visible surfaces, although this is usually secondary for a mold base.
Electroless Nickel Plating
Electroless nickel plating, often abbreviated as ENP, deposits a nickel-phosphorus alloy without the use of an electric current. The process is autocatalytic and produces a uniform coating on complex geometries, including internal water lines, pockets, and recessed areas. Typical thickness is 10 to 50 micrometres. High-phosphorus ENP, generally with 10 to 13 percent phosphorus, provides the best corrosion resistance in cooling water circuits.
ENP is one of the most useful treatments for die-casting mold base plates in humid environments. It is particularly valuable for A-plates and B-plates with water lines close to the base material, because it can protect the internal channels as well as the exterior. The coating is uniform and does not build up heavily on edges in the way that some electroplated coatings can. As-plated hardness is around 500 HV, and after a suitable heat treatment it can reach approximately 1000 HV, although heat treatment must be controlled to avoid affecting the base plate.
ENP is not a cure-all. Good pretreatment is essential. The surface must be clean, activated, and free from oil, rust, and machining residue. Threads, dowel holes, and precision bores must be masked or allowed for, because even a uniform coating changes dimensions. The process should be specified with the required phosphorus content, thickness, hardness, and corrosion test. For sliding applications, ENP with PTFE can be used to provide self-lubricating properties.
Hard Chrome Plating
Hard chrome plating is an electroplated chromium layer with high hardness, typically in the range of 800 to 1000 HV. Typical thickness for mold base applications is about 10 to 40 micrometres, although thicker deposits are possible. It provides good abrasion resistance and moderate corrosion resistance. It is usually applied selectively to wear surfaces, clamping slots, platen-facing plates, wear plates, and areas that experience sliding or impact.
Hard chrome is not normally applied to an entire large base plate. It is expensive, it requires grinding or lapping after plating, and it can build up unevenly at sharp edges. The process can also introduce hydrogen into the steel, so hydrogen embrittlement relief may be required for high-strength or highly stressed components. The need for baking should be discussed with the plating supplier. Hard chrome is best used as a targeted treatment where wear resistance is more important than uniform corrosion protection.
Zinc Plating and Paint
Zinc plating and galvanizing are cheaper corrosion-protection methods. They are sometimes used on low-end base plates, ejector plates, or non-critical components. Zinc coatings can provide useful sacrificial protection, but they are generally less durable than ENP or QPQ in a die-casting environment, and they may not be suitable for precision sliding surfaces. Zinc plating should not be specified for critical water lines unless the process and corrosion performance have been validated.
Paint is another option for non-machined exterior surfaces. Blue, green, or grey anti-rust paint is often applied to the outside faces of mold bases. Paint should not be applied to mating surfaces, guide bores, water-line sealing faces, or precision locating surfaces. The paint specification should include surface preparation, primer, topcoat, and masking requirements. Paint improves appearance and exterior corrosion resistance, but it does not protect internal water lines or sliding surfaces.
Wear and Galling Resistance Treatments
Gas and Plasma Nitriding
Nitriding is one of the most common wear treatments for mold base components. In gas nitriding or plasma nitriding, nitrogen is diffused into the steel surface at a temperature typically between 500 and 550 degrees Celsius. This creates a hard case with a depth usually between 0.1 and 0.3 millimetres and a hardness in the range of 600 to 800 HV, or roughly 60 to 70 HRC depending on the steel and process.
Nitriding is used on guide pin holes, leader pin bores, ejector guide holes, clamping faces, and high-load support plates. It reduces wear and helps prevent local brinelling under clamping loads. When controlled correctly, distortion is minimal, but it is not zero. The treated surface grows slightly, and the case depth must be considered when tight tolerances are required. Some processes may leave a white layer or compound zone that can be brittle; this may need to be controlled or removed depending on the application.
Nitriding is most effective on alloy steels that contain nitride-forming elements such as chromium, molybdenum, and aluminum. P20, 4140, and H13 respond well. S50C carbon steel can be nitrided, but the hardness and case quality are generally lower, so nitrocarburizing or another treatment may be more appropriate. Nitriding should be performed after rough machining and stress relief, and the final dimensional allowances must be planned before the process. If the plate is nitrided after final machining, the growth must be accounted for, or the critical bores may need post-treatment lapping.
Nitrocarburizing and QPQ
Nitrocarburizing introduces both nitrogen and carbon into the surface. It produces a thin compound zone, typically about 10 to 20 micrometres, supported by a deeper diffusion zone. The compound zone provides high surface hardness, good corrosion resistance, and a low coefficient of friction. QPQ, which stands for quench-polish-quench, is a well-known nitrocarburizing process that includes polishing and oxidation steps. It is also known by trade names such as Tenifer, Tufftride, and Melonite.
QPQ is a strong candidate for export base plates and long-storage molds because it combines wear resistance with a black corrosion-resistant finish. It is commonly used on guide components, slide retainers, small base plates, ejector guide bushings, and wear plates. The dimensional change is relatively low, but it is not zero. The compound zone and diffusion zone must be specified, and critical tolerances should be agreed with the heat treater. Salt-bath QPQ processes require environmental controls and waste treatment, so the supplier should be qualified for the process.
PVD Coatings
PVD, or physical vapor deposition, is a vacuum coating process that applies thin, hard ceramic or carbon films to a steel surface. Common PVD coatings include titanium nitride, chromium nitride, and other nitride or carbide layers. Typical thickness is only about 2 to 5 micrometres, but the hardness can exceed 2000 HV. PVD coatings are used on cavity support faces, sliding areas, wear plates, gibs, and ejector guide bushings where high clamping pressure, flashing, or friction is a concern.
PVD is rarely applied to a complete large base plate because vacuum chamber size is limited and the process is line-of-sight. It is much more practical to coat bolted-on wear plates, small inserts, and replaceable guide components. PVD also requires a suitable substrate and good surface preparation. If the base material is soft or poorly supported, a thin hard coating may not prevent substrate deformation. PVD should therefore be used as part of a system that includes adequate base hardness and support.
DLC Coatings
DLC, or diamond-like carbon, is a thin coating with low friction and good anti-galling properties. It is often used on moving components in the base, such as ejector guides, sliding plates, and wear surfaces that must operate with minimal lubrication. DLC is more expensive than many other treatments, and it is not normally applied to large base plates. It is best reserved for specific high-friction or low-lubrication locations where its low friction and wear resistance justify the cost.
Electroless Nickel with PTFE
Electroless nickel with PTFE, sometimes called nickel-Teflon, is a self-lubricating version of ENP. The PTFE particles are co-deposited in the nickel matrix, reducing friction and improving release and sliding behaviour. It is used on ejector guide holes, slider pockets, and other sliding areas where oil retention is difficult or where a low-friction surface is needed. It offers the corrosion protection of ENP plus lubricity, but it is not a substitute for a hard wear coating in high-load applications.
Surface Conditioning and Stress Management
Shot Peening and Blasting
Shot peening and glass bead blasting are surface conditioning processes rather than protective coatings. Shot peening induces compressive residual stresses on machined pockets, fillets, and sharp corners. This can improve fatigue resistance under high-tonnage clamping forces. Glass bead blasting creates a uniform matte finish and can be used to clean or prepare a surface before coating.
These processes must be specified carefully. Excessive peening can distort thin sections, and blasting can change surface roughness and dimensional tolerance if not controlled. They are usually performed before final coating or before final assembly. A uniform matte finish may also improve the appearance of non-critical surfaces and help oil retention.
Final Grinding and Stress Relief
Final grinding is not a surface treatment in the chemical sense, but it is part of the surface condition that determines mold base performance. Double-side grinding can achieve parallelism values in the range of 0.02 millimetres, which is important for clamping stability and insert seating. Stress relief after rough machining helps reduce dimensional movement during subsequent machining and heat treatment.
The sequence must be planned. A typical sequence is rough machining, stress relief, semi-finish machining, heat treatment if required, finish machining, surface treatment, and final inspection. If a coating is applied before final grinding, the grinding will remove it from critical surfaces. If a coating is applied after final grinding, the coating thickness and any surface growth must be allowed for. This is one of the most common sources of confusion in mold base purchasing.
Comparison of Common Base Plate Treatments
| Treatment | Typical thickness | Primary purpose | Dimensional impact | Best used on | Main limitations |
|---|---|---|---|---|---|
| Black oxide | 1 to 3 micrometres | Basic rust prevention and cosmetic finish | Negligible | Exterior plate faces, clamping plates, general machined surfaces | Short-term protection, poor for water lines, little wear resistance |
| Phosphate | 2 to 10 micrometres | Oil retention and anti-rust for storage and shipment | Low | Exterior surfaces, plates for sea shipment, storage | Not a wear coating, removed by final grinding if applied too early |
| Electroless nickel | 10 to 50 micrometres | Corrosion protection inside and outside | Uniform buildup, must be allowed for in bores and threads | Water-cooled A and B plates, humid shops, complex geometries | Pretreatment critical, masking required, not ideal for high-load wear unless heat treated |
| Hard chrome | 10 to 40 micrometres | Abrasion and moisture resistance | Uneven at edges, often requires grinding | Wear plates, clamping slots, platen-facing surfaces | Selective use, hydrogen embrittlement risk, not for whole large plates |
| Gas or plasma nitriding | 0.1 to 0.3 millimetres case depth | Surface hardness and anti-galling | Small growth, must be allowed for | Guide pin holes, leader pin bores, ejector guides, clamping faces | Distortion risk if uncontrolled, white layer control, best on alloy steels |
| QPQ or nitrocarburizing | 10 to 20 micrometres compound zone | Combined wear and corrosion resistance | Low | Guide components, slide retainers, small plates, export molds | Salt-bath environmental controls, compound zone control |
| PVD TiN or CrN | 2 to 5 micrometres | High hardness and low friction | Very low, but line-of-sight | Wear plates, gibs, ejector guide bushings, sliding details | Chamber size limits, not for massive base plates, requires good substrate |
| DLC | 1 to 5 micrometres | Low friction and anti-galling | Very low | Moving components, ejector guides, low-lubrication sliding surfaces | High cost, limited to specific components |
| Zinc plating | 5 to 15 micrometres | Low-cost corrosion protection | Low to moderate | Low-end bases, ejector plates, non-critical parts | Less durable, not for precision sliding or critical water lines |
| Paint | 20 to 80 micrometres or more | Exterior appearance and corrosion protection | Can affect fit if applied to mating surfaces | Non-machined exterior faces | Must be masked, no protection inside water lines |
Selection Guide by Application
Budget and Fast Turnaround
For a mold that will be used quickly in a dry shop, the most economical choice is often final grinding plus black oxide. This provides basic rust prevention during machining, assembly, and short-term storage. It is not the best choice for humid environments or long shipment, but it is practical for many domestic molds with a short lead time. A rust-preventive oil should be applied before storage.
Export and Long Storage
For export or long storage, black oxide alone is usually not enough. Phosphate coating with oil, or QPQ, offers better corrosion protection. Phosphate is cost-effective and improves oil retention. QPQ provides a harder surface and a black corrosion-resistant finish, which is attractive for high-value export base plates. VCI packaging and desiccant can be added for additional protection. Water lines should be dried and plugged, and the internal condition should be inspected before shipment.
Humid Shop and Water Lines
In a humid die-casting shop, water-line corrosion is a major concern. High-phosphorus electroless nickel is often the best choice for A-plates and B-plates with cooling channels because it deposits uniformly inside the channels. The phosphorus content, coating thickness, and corrosion test should be specified. Hard chrome can be used selectively on wear surfaces, but it is not a substitute for internal water-line protection. If the water chemistry is aggressive, the mold designer should also consider water treatment, flow rate, and channel cleaning, because no coating can compensate for poor water quality.
High-Cycle and Heavy Clamping
For high-cycle molds and heavy clamping loads, nitriding is a common choice for guide pin holes, leader pin bores, ejector guide holes, and clamping faces. It improves wear resistance and reduces brinelling. QPQ can be used on smaller guide components and slide retainers. Hard chrome can be applied to wear plates and clamping slots. A combination such as nitriding on the plate plus black oxide on non-critical exterior surfaces is often practical and cost-effective.
Precision and Low-Friction Sliding
For precision sliding, PVD, DLC, QPQ, and ENP with PTFE are all possible. PVD and DLC are usually applied to replaceable wear plates and guide components rather than to the whole base plate. QPQ is useful where both wear and corrosion resistance are needed. ENP with PTFE is useful where oil retention is difficult. The choice depends on load, speed, lubrication, and the cost of replacing the component.
Material Considerations: S50C, P20, 4140, and H13
S50C or 1050 carbon steel is a common base plate material for standard molds. It is relatively economical and easy to machine. Black oxide, phosphate, zinc plating, and paint are common treatments. Nitriding is possible but less effective than on alloy steels, so nitrocarburizing or QPQ may be preferred when wear resistance is required. S50C is often used for ejector plates and less highly loaded base plates.
P20 or 1.2311 is a pre-hardened alloy steel widely used for mold bases. It responds well to nitriding, ENP, black oxide, and QPQ. Nitriding can be used on guide pin holes and clamping faces, but the process temperature and time must be controlled to avoid softening the pre-hardened substrate. P20 is a good general-purpose material for die-casting mold bases when the loads are moderate.
4140 is a chromium-molybdenum alloy steel with good strength and hardenability. It responds well to nitriding, QPQ, and hard chrome. It is often used for support plates, wear plates, and highly loaded base components. H13 is a hot-work tool steel with excellent temper resistance and nitriding response. In a mold base, H13 may be used for support pillars, wear details, or areas close to the cavity where heat exposure is higher. Nitriding and QPQ are both suitable for H13, but the heat treatment history and final hardness must be considered.
The material choice and surface treatment should be specified together. A treatment that works well on H13 may not perform the same way on S50C. A coating that requires a hard substrate may fail on a soft base plate. The mold designer should not separate the base material specification from the surface treatment specification.
Specifying Treatments on Drawings and Purchase Orders
A useful surface treatment specification should include the process name, the areas to be treated, the areas to be masked, the required thickness or case depth, the required hardness, the dimensional allowance, the surface preparation, and the inspection method. For electroless nickel, specify the phosphorus content and whether heat treatment is required. For nitriding, specify the case depth, surface hardness, and acceptable white layer. For QPQ, specify the compound zone and diffusion zone. For hard chrome, specify the thickness and the grinding allowance. For black oxide and phosphate, specify the rust-preventive oil or wax.
The purchase order should also define the sequence. If the plate is to be final ground after coating, the coating on the ground surfaces will be removed. If the plate is to be coated after final grinding, the coating thickness must be allowed for. Threads, dowel holes, water-line ports, and sealing faces should be masked as required. The supplier should provide a process route and a inspection plan before production.
Inspection and Quality Control
Inspection should match the criticality of the mold base. Common checks include visual inspection, coating thickness measurement, hardness testing, case-depth measurement, adhesion testing, salt-spray or corrosion testing, and dimensional inspection. For nitrided plates, case depth and surface hardness are important. For ENP, thickness, phosphorus content, and corrosion resistance should be verified. For hard chrome, thickness and adhesion should be checked. For QPQ, the compound zone and surface appearance should be controlled.
Dimensional inspection is especially important because coatings can change bore sizes and flatness. Critical bores should be measured before and after treatment. Water lines should be checked for blockage or excessive coating buildup. Threads should be checked with gauges. If the plate is large, flatness and parallelism should be measured after treatment, not only after machining.
Common Mistakes and How to Avoid Them
One common mistake is to specify a high-end coating for the entire base plate when only a small wear area needs protection. PVD and DLC are rarely practical for a complete A-plate or B-plate. Another mistake is to rely on black oxide for water-line corrosion protection. Black oxide is a short-term exterior finish, not a solution for aggressive cooling channels.
A third mistake is to apply nitriding without allowing for dimensional growth. Guide pin bores and ejector guide holes can become too tight after treatment. A fourth mistake is to apply a coating after final grinding without considering thickness. Precision bores and sealing faces may no longer meet tolerance. A fifth mistake is to paint mating surfaces or guide bores. Paint should be restricted to non-machined exterior faces.
Finally, the process sequence should not be left to chance. Stress relief, rough machining, heat treatment, finish machining, surface treatment, and final inspection must be planned as a system. The supplier should confirm the sequence in writing, especially when multiple treatments are combined.
FAQ
Which surface treatment is most common for die-casting mold base plates?
Black oxide is the most common low-cost default for general machined surfaces. It provides basic rust prevention, improves appearance, and has almost no dimensional impact. For wear resistance, nitriding and QPQ are more common. For water-line corrosion, electroless nickel is often preferred.
Can electroless nickel be applied inside cooling channels?
Yes, electroless nickel can coat internal water lines if the channels are accessible to the plating solution and properly cleaned. High-phosphorus ENP is preferred for corrosion resistance. The supplier must confirm that the channel geometry, length, and connections allow adequate solution flow. Thickness and masking should be specified.
Is nitriding suitable for P20 and H13 base plates?
Yes. Both P20 and H13 can be nitrided, but the process must be controlled. H13 generally responds better to nitriding because of its alloy content. P20 is pre-hardened, so the nitriding temperature and time should avoid excessive softening. Dimensional growth and white-layer control should be specified.
Should I choose black oxide or phosphate for sea shipment?
Phosphate with rust-preventive oil is usually better than black oxide for sea shipment because it retains oil and provides better temporary protection. QPQ is an even stronger choice when wear resistance and corrosion resistance are both required. Black oxide alone is usually not sufficient for long humid shipment unless additional packaging protection is used.
Can PVD or DLC coat a large mold base plate?
PVD and DLC are rarely applied to a complete large base plate because of vacuum chamber size and line-of-sight limitations. They are more commonly used on wear plates, gibs, ejector guide bushings, and small sliding components. The base plate itself is usually protected by black oxide, phosphate, ENP, nitriding, or QPQ.
What should be written on the drawing for surface treatment?
The drawing should state the process, treated areas, masked areas, thickness or case depth, hardness, dimensional allowance, surface preparation, and inspection method. For nitriding, specify case depth and white-layer acceptance. For ENP, specify phosphorus content and heat treatment. For hard chrome, specify thickness and grinding allowance. For black oxide or phosphate, specify the protective oil.
Conclusion
Surface treatment of die-casting mold base plates is a functional decision. The base plate does not usually face molten metal, so the treatment should target the real failure modes: corrosion from cooling water and humidity, wear and galling on guide and ejector components, and dimensional stability under repeated clamping. The best treatment is the one that matches the material, the environment, the feature being protected, and the required tolerance.
For general-purpose molds, ground and black-oxided plates are often sufficient. For export or long storage, phosphate with oil or QPQ provides better protection. For humid shops and water-cooled plates, high-phosphorus electroless nickel is a strong choice. For high-cycle clamping and guide wear, nitriding and QPQ are effective. For precision sliding, PVD, DLC, QPQ, and ENP with PTFE can be used selectively on wear plates and guide components. Hard chrome remains useful for targeted abrasion resistance, while zinc plating and paint are best limited to non-critical surfaces.
The key is to specify the treatment before final machining, allow for coating thickness or case growth, mask critical features, and inspect the result. When the treatment is planned as part of the manufacturing route rather than added at the end, die-casting mold base plates can achieve better corrosion resistance, longer service life, and more reliable dimensional performance.