Introduction
The question sounds simple, but in die-casting tooling it hides an important distinction. A die-casting mold is not one homogeneous block of hardened steel. It is an assembly. The mold base—the plates, frame, bolsters, support blocks, ejector plates, guide-pin bores, and mounting features—holds the active tooling and carries the clamp loads. The cavity, core, slides, and inserts—the forming parts—contact molten metal and therefore need a different steel and heat treatment. The base is structural; the inserts are thermal and wear components. Treating them as one specification is one of the most common causes of over-hardened, cracked, difficult-to-machine, or dimensionally unstable mold bases.
The short answer is that a standard die-casting mold base is normally supplied pre-hardened to approximately 28–36 HRC, with 30–34 HRC being the most commonly quoted working range. It should be stress-relieved after rough machining, usually in the range of 600–680°C for structural and medium-carbon grades, or around 500–550°C for many pre-hardened P20/718-type plates, depending on the steelmaker’s original tempering temperature. The exact cycle should always be tied to the steel grade and the amount of stock removed. The base should not normally be through-hardened to 44–48 HRC. That is cavity-insert territory.
This article explains the typical hardness and stress-relief condition, why those values are chosen, how to specify them, how to inspect them, and where the exceptions lie.
The two zones of a die-casting tool
Mold base
The mold base is the frame. It includes the clamp plates, cavity plates, core plates, support plates, ejector housings, ejector plates, guide pillars and bushings, return pins, support pillars, and sometimes slides and wedges. It transmits the clamping force from the machine to the parting line, keeps the cavity and core aligned, carries the ejector system, and provides mounting and handling features. It does not see molten aluminum, zinc, or magnesium at the cavity surface. It does see high compressive stress, bending, wear at guide components, and repeated clamping.
Forming parts
The forming parts include cavity inserts, cores, slides, and small inserts that form the part. These are made from hot-work tool steels such as H13, SKD61, 1.2344, 8407, or Dievar, and are hardened and tempered to a much higher hardness, commonly 43–48 HRC. For aluminum die casting, many specifications target 46–48 HRC, and some companies set a minimum of about 47 HRC for forming surfaces to resist heat checking, erosion, and cracking. These parts also require periodic stress relief in service, often after the first production run and then at intervals such as every 10,000 shots, depending on the alloy, die temperature, and shot weight.
The distinction matters because the mold base is designed for machinability, structural stiffness, and dimensional stability, not for resistance to molten-metal erosion. A base at cavity hardness is not a better base. It is usually a more brittle, more difficult-to-machine, and more crack-prone base.
What hardness should a mold base normally have?
Standard working range
For a conventional die-casting mold base, the typical hardness is 28–36 HRC. In commercial practice, many mold-base suppliers quote 30–34 HRC for pre-hardened P20-type plates. Some classification guides put standard LME-type bases at 28–32 HRC and frame plates at 30–36 HRC. The exact value depends on the plate size, steel grade, supplier, and whether the plate is a cavity plate, core plate, support plate, or ejector plate.
A practical range for a general-purpose base is:
| Mold-base element | Typical hardness | Comment |
|---|---|---|
| Cavity and core plates | 30–36 HRC | Pre-hardened P20/718/1.2738 type |
| Frame and clamp plates | 28–34 HRC | Structural, pre-hardened or normalized |
| Support plates | 28–34 HRC | Stiffness is more important than wear resistance |
| Ejector plates | 25–32 HRC | Often softer for machining and pin bores |
| Guide pillars and bushings | 50–60 HRC or surface-hardened | Wear components, not the base plate itself |
| High-life through-hardened base | 38–44 HRC | Exception, not the standard |
The common base steels include P20, 1.2311, 1.2738, 718, 4140, and S50C or 1.1730. P20, 1.2311, 1.2738, and 718 are typically supplied pre-hardened in the 28–36 HRC range. 4140 can be supplied pre-hardened or quenched and tempered to a similar range. S50C and 1.1730 are medium-carbon structural steels that may be supplied in a softer, normalized or annealed condition where the load and wear conditions allow. That is why a single number cannot be applied blindly to every plate. The specification should say the actual grade and the required hardness range, not just the word hard.
Why this range is chosen
The 28–36 HRC range is a compromise between three requirements.
First, machinability. Mold bases require extensive milling, drilling, tapping, boring, and sometimes deep-pocket machining. At 28–36 HRC, the steel can be cut with standard carbide tooling at reasonable feeds and speeds. At 44–48 HRC, tool life drops, tapping becomes difficult, and the risk of cracking around bolt holes and guide-pin bores increases. The base has many holes and pockets; it is not a simple cavity block.
Second, structural strength. The base must resist compression under clamping force and injection pressure, support the cavity inserts, and maintain alignment. A hardness of 28–36 HRC gives sufficient yield strength and resistance to indentation for most die-casting bases. The stiffness comes mainly from section thickness and support pillars, not from hardness. Hardness helps with local bearing and wear, but it cannot compensate for an under-designed support system.
Third, dimensional stability and toughness. A moderately hard, pre-hardened base is tough enough to tolerate stress concentrations at holes and corners. A very hard base is more sensitive to cracking, especially if it is not stress-relieved properly. Since the base does not see molten-metal erosion, there is little technical benefit in pushing it to cavity hardness.
Why not harden the base to cavity hardness?
If a mold base is specified at 44–48 HRC, several problems follow. Machining becomes slower and more expensive. Tapping and deep-hole drilling become risky. Bolt holes and leader-pin holes can become crack initiation sites. The base becomes less forgiving of minor design or manufacturing errors. And the benefit is small, because the base does not contact molten metal. A hard base does not reduce heat checking, erosion, or soldering; those are functions of the cavity insert material and surface treatment.
There is also a common commercial confusion: a supplier may quote a base at 44–48 HRC because they are actually quoting cavity steel or cavity heat treatment. If the purchase order says mold base and the quotation says 44–48 HRC for all plates, the buyer should ask for clarification. The base and the inserts should be listed separately.
Exceptions
There are exceptions. For very high shot life, some suppliers use H13 or 718 pre-hardened to 38–44 HRC for the base, or through-harden certain wear plates. This is not the standard base. It may be justified for high-volume tools, aggressive clamping, or special wear conditions. Even then, the design should be reviewed for toughness and stress relief, and the hardness should be specified by plate function, not applied to the entire assembly. Guide pillars, bushings, and wear plates may be hardened to 50–60 HRC or surface-hardened, but those are separate components, not the structural base plates.
Stress relief: the condition that matters as much as hardness
Where residual stress comes from
A mold base begins with residual stress from steelmaking, forging, rolling, and the supplier’s heat treatment. Additional stress is introduced by machining: rough milling removes large amounts of material from one side of a plate, deep pockets create unbalanced sections, large holes interrupt the stress field, and surface grinding can introduce a shallow stress layer. Welding repairs, EDM, and even heavy clamping can add stress. If these stresses are not relieved, the plate may warp during final machining, during heat treatment, or in service. A warped base can cause flashing, parting-line mismatch, guide-pin binding, uneven clamping, and premature wear.
Stress relief is therefore not optional for a precision die-casting mold base. It is a process step that stabilizes the plate before final finishing. The goal is not to soften the base. The goal is to reduce residual stress while keeping the hardness within the specified working range.
Recommended stress-relief sequence
A robust sequence for a precision mold base is:
- Raw material verification. Confirm the steel grade, hardness, and ultrasonic or surface condition as required. For large plates, check for laminations or internal defects.
- Pre-machining stress relief if needed. If the plate has been flame-cut, forged, or heavily straightened, a stress-relief anneal or normalizing and tempering cycle may be required before rough machining.
- Rough machining. Remove most of the stock, typically 70–80 percent of the material to be removed. Leave enough allowance for final machining, but do not leave so much that the final cut is the first major cut.
- First stress relief after rough machining. This is the most important cycle for the base. Heat the plate uniformly, hold at temperature, and cool slowly and uniformly.
- Semi-finish machining. Bring the plate closer to final dimensions, leaving a small allowance for finishing.
- Second stress relief or stabilization before finish machining. This is common for large, thin, or high-precision bases. It reduces the stress introduced by semi-finishing and helps hold flatness and parallelism.
- Final machining and grinding. Use light cuts and symmetrical material removal where possible.
- Inspection. Check hardness, flatness, parallelism, and critical dimensions. Record the results.
In practice, some shops also rough to remove most of the stock and then let the plate sit for 12–48 hours before finishing. This is not a substitute for a proper stress-relief cycle, but it can allow some residual stress to relax and can reveal movement before the final cut.
Practical temperature windows and cycles
There is no single stress-relief temperature for all mold-base steels. The correct cycle depends on the steel grade, the original heat treatment, the hardness specification, and the amount of machining stress. Two ranges are commonly encountered.
For medium-carbon and structural grades such as S50C, 1.1730, and 4140 in the pre-hardened or quenched-and-tempered condition, stress relief is often performed in the 600–680°C range. A typical cycle is: heat uniformly to 650–680°C, hold for 2–4 hours, and cool in air or in a controlled furnace. For thick plates, the hold time is often estimated as about one hour per 25 mm of section thickness, with a minimum of two hours. The exact cycle should be confirmed with the steel supplier.
For pre-hardened P20, 1.2311, 1.2738, and 718-type plates, the stress-relief temperature must be kept below the original tempering temperature to avoid reducing the hardness. Many suppliers recommend a stress-relief or stabilization cycle around 500–550°C for these grades, although some specifications use somewhat higher or lower temperatures depending on the grade and the required hardness. A common specification for pre-hardened plates is to stress relieve after rough machining at a temperature about 30–50°C below the original tempering temperature, hold for two to four hours, and cool slowly. This is why a generic instruction such as heat to 650°C can be wrong for a pre-hardened P20 base: it may soften the plate below the specified hardness.
The first model answer quoted a range of 480–550°C, and the second quoted 650–680°C. Both can be correct for different steel conditions. The practical rule is: match the stress-relief cycle to the steel grade and the original tempering temperature. For a pre-hardened P20/718 base, use the steelmaker’s recommended stress-relief temperature, often around 500–550°C. For a structural 4140 or medium-carbon base that is not sensitive to tempering back, a 600–680°C stress-relief anneal may be appropriate. Never use a stress-relief temperature that exceeds the final tempering temperature of a pre-hardened plate unless the hardness specification allows it.
Cooling should be uniform. Small plates may be air-cooled. Large or complex plates should be furnace-cooled or covered to avoid thermal gradients. Rapid cooling can introduce new residual stress and defeat the purpose of the cycle.
Roughing, stabilization, and finishing strategy
The most reliable way to hold a mold base flat is to plan the machining sequence around stress relief, not to try to machine around stress after it appears. A good sequence removes stock symmetrically, relieves stress after roughing, and leaves only a small amount of material for final machining. Deep pockets should be roughed from both sides where possible, or the plate should be stress-relieved after the first side is roughed. If a large pocket removes most of the section on one side, the plate will often bow toward the remaining material. Stress relief after that roughing step is essential.
For large bases, it is common to leave 0.5–1.5 mm of stock for final machining after stress relief. The exact allowance depends on plate size, distortion risk, and the capabilities of the machine shop. The final finishing cuts should be light and should not remove more material than necessary. If a base is stress-relieved after roughing and then heavily machined again, a second stabilization cycle before final grinding is good practice.
How to specify hardness and stress relief on a purchase order
A clear purchase order prevents most disputes. A good specification should state the material, the hardness range for each plate, the stress-relief cycle, the inspection method, and the dimensional requirements. It should not simply say mold base, hardened, or stress relieved.
A practical purchase-order note for a standard die-casting mold base is:
Base material: P20 pre-hardened or 4140, 30–34 HRC for cavity and core plates; 28–34 HRC for frame and support plates; ejector plates 25–32 HRC unless otherwise specified. Stress relieve after rough machining at 500–550°C for pre-hardened P20/718-type plates, or 600–680°C for structural grades, hold 2–4 hours, cool uniformly. Provide hardness certificate with test locations and stress-relief record. Final flatness and parallelism to drawing; critical plates to be checked after finish grinding.
For a high-life tool, the note might add: through-hardened or H13 base plates at 38–44 HRC only where specified; guide pillars and bushings heat-treated separately to 50–60 HRC or surface-hardened. For a large base, add: ultrasonic inspection of critical plates; flatness measured after stress relief and after final machining; no welding repair without approval and subsequent stress relief.
The specification should also state what is not required. For example: do not through-harden standard base plates to cavity hardness; do not stress relieve finished guide-pin bores at a temperature that will distort them; do not grind after stress relief without a stabilization check if the plate is large.
Inspection and acceptance
Hardness inspection should be done on a clean, decarburization-free surface. Portable Leeb hardness testers are common, but they should be correlated with Rockwell or Brinell readings for the specific material. For critical plates, use a bench hardness tester or a calibrated portable device. Take multiple readings at different locations, especially on large plates, and record the test locations. Hardness can vary across a large plate, and a single reading is not sufficient.
Stress relief is harder to inspect directly because residual stress is not visible. The acceptance evidence is the process record: furnace chart, holding time, temperature, cooling method, and the steel grade. For critical tools, witness coupons or dimensional checks before and after stress relief can be used. Flatness and parallelism should be measured after rough machining, after stress relief, and after final machining. A plate that moves during final machining is a warning sign that the stress-relief cycle was inadequate or that too much stock was removed after stress relief.
Typical flatness requirements depend on the mold size and the part tolerance. For a precision base, a flatness of 0.02–0.05 mm over a 300 mm span is often targeted, with tighter values for small precision tools and looser values for large structural plates. Parallelism between the clamp faces and the parting line is equally important. The exact tolerance should be on the drawing, because a base that is flat but not parallel will still produce uneven clamping and flashing.
Mold base versus cavity inserts: a comparison
The following comparison summarizes the difference:
| Item | Mold base | Cavity inserts |
|---|---|---|
| Function | Structure, alignment, clamping, ejection | Forming surface, molten-metal contact |
| Common steel | P20, 1.2311, 1.2738, 718, 4140, S50C, 1.1730 | H13, SKD61, 1.2344, 8407, Dievar |
| Typical hardness | 28–36 HRC, often 30–34 HRC | 43–48 HRC, often 46–48 HRC for aluminum |
| Heat treatment | Pre-hardened, stress relieved | Hardened and tempered, sometimes nitrided |
| Main failure modes | Warpage, wear, cracking at holes, misalignment | Heat checking, erosion, cracking, soldering |
| Stress relief | After rough machining, sometimes before finish | In service at intervals, often around 10,000 shots |
The comparison makes the answer to the original question clearer. A die-casting mold base is not supposed to reach cavity hardness. It is supposed to be strong enough, tough enough, stable enough, and machinable enough to hold the cavity system in alignment. The cavity inserts are the parts that need high hardness and resistance to thermal fatigue.
Application notes for aluminum, zinc, and high-life tools
For aluminum die casting, the thermal load on the cavity is high, and the forming inserts are usually specified at 46–48 HRC. The mold base, however, remains a structural component. The base may be made from P20 or 718 pre-hardened to 30–36 HRC, with stress relief after roughing. If the tool is large or has deep pockets, a second stress relief before finishing is recommended. The base should be designed with adequate support pillars and sufficient plate thickness, because aluminum die casting often uses high injection pressures and high clamping forces.
For zinc die casting, the molten-metal temperature is lower than for aluminum, but the tooling still requires proper stress relief and alignment. The base hardness range is similar. For magnesium, the process environment and safety requirements are different, but the base remains structural; the cavity inserts and surface treatments are the main wear and thermal considerations.
For high-life tools, some customers specify through-hardened base plates or H13 base plates at 38–44 HRC. This can be justified for very high shot counts or severe wear conditions, but it should be a deliberate exception. The designer should check that the higher hardness does not create cracking risk at holes and corners, and the heat treater should use a stress-relief cycle that matches the final hardness. In most cases, a properly designed 30–34 HRC base with good support and stress relief will outperform an over-hardened base with poor toughness.
Common mistakes and how to avoid them
The first mistake is specifying the same hardness for the base and the cavity. This leads to unnecessary machining cost and cracking risk. Separate the two specifications.
The second mistake is skipping stress relief after rough machining. A base that is machined from a stressed plate can move during final machining or in service. Plan the stress-relief step into the route card.
The third mistake is using a stress-relief temperature that is too high for a pre-hardened plate. This can soften the base below the specified hardness. Use the steelmaker’s data and record the cycle.
The fourth mistake is stress-relieving after final machining without allowing for distortion. If a finished base is heated, it may move. Stress relief should be done before final finishing, with enough allowance to correct any movement.
The fifth mistake is ignoring the guide-pin and bushing alignment. The base may be hard enough, but if the guide-pin bores are not aligned and stress-relieved properly, the mold will bind. Check alignment after stress relief and after final machining.
The sixth mistake is using welding to repair a base without subsequent stress relief. Welding introduces local stress and can cause cracking or movement. If welding is necessary, use a controlled procedure and stress-relieve afterward.
FAQ
Is 30 HRC strong enough for a die-casting mold base?
Yes, for most standard die-casting bases. The base carries compressive and bending loads, but it does not contact molten metal. At 30–34 HRC, pre-hardened P20 or 718 has sufficient strength for normal clamping and injection pressures, provided the plate thickness and support pillars are correctly designed. The stiffness of the base comes mainly from its section and support system, not from a high hardness number. If the tool is very large or the clamping loads are unusually high, the design should be reviewed rather than simply increasing hardness.
Should a mold base be through-hardened to 45 HRC?
No, not as a standard practice. A 45 HRC base is closer to cavity-insert hardness and brings problems: reduced machinability, difficult tapping, higher cracking risk at holes and corners, and little functional benefit because the base does not see molten-metal erosion. A 44–48 HRC quotation for a standard base usually means the supplier is quoting cavity steel or cavity heat treatment. Through-hardened bases at 38–44 HRC exist for special high-life applications, but they are exceptions and should be specified deliberately.
What stress-relief temperature should be used after rough machining?
It depends on the steel. For structural and medium-carbon grades such as 4140 or S50C, a stress-relief anneal around 600–680°C, held for 2–4 hours and slow-cooled, is common. For pre-hardened P20, 1.2311, 1.2738, or 718 plates, use a temperature below the original tempering temperature, often around 500–550°C, and follow the steelmaker’s recommendation. A hold time of about one hour per 25 mm of thickness, with a minimum of two hours, is a practical starting point. The key is to avoid softening the plate or introducing new thermal stress.
How many stress-relief cycles does a precision mold base need?
At least one after rough machining. For large, thin, deep-pocketed, or high-precision bases, a second stabilization cycle before finish machining is common. If the base is welded, heavily machined after the first stress relief, or expected to hold tight flatness, a second cycle is good practice. The exact number should be based on the amount of residual stress and the dimensional tolerance, not on a fixed rule.
What hardness should the cavity inserts have?
Cavity inserts, cores, and slides for die casting are usually made from H13-type hot-work steel and hardened to 43–48 HRC. For aluminum die casting, many specifications target 46–48 HRC, and some companies require at least 47 HRC on forming surfaces to resist heat checking and cracking. These parts also need periodic stress relief in service, often after the first production run and then at intervals such as every 10,000 shots. The mold base should not be confused with these inserts.
How can I verify that the supplier has stress-relieved the base?
Ask for the process record: furnace chart, holding temperature, holding time, cooling method, and the steel grade. Ask for hardness certificates with test locations. Check flatness and parallelism after stress relief and after final machining. For critical tools, require dimensional inspection before and after stress relief, or witness the cycle. A supplier who cannot provide a stress-relief record is a risk for precision bases.
Conclusion
A die-casting mold base should normally be supplied pre-hardened to about 28–36 HRC, with 30–34 HRC being the most common working range for P20, 1.2311, 1.2738, 718, and 4140-type plates. It should be stress-relieved after rough machining, using a cycle that matches the steel grade: often 600–680°C for structural grades, or around 500–550°C for pre-hardened plates where the original tempering temperature requires it. A second stabilization cycle before finish machining is good practice for precision or large bases. The base should not normally be through-hardened to cavity-insert hardness. Cavity inserts are different: H13-type hot-work steels at 43–48 HRC, often 46–48 HRC for aluminum, with periodic stress relief in service.
The practical specification is therefore not a single number. It is a combination of material, hardness range by plate function, stress-relief cycle, machining sequence, and inspection. When those elements are specified clearly, the mold base will be strong enough, stable enough, and machinable enough to support the cavity system for the life of the tool. When they are not, the result is often a base that is harder than necessary, more expensive than necessary, and less reliable than a properly stress-relieved standard base.
参考资料
- The Reasons For Aluminum Die Casting Tooling Easy Cracking
- https://tooling.harsle.com/the-ultimate-revelation-of-die-casting-mold/
- https://moldiecasting.com/blog/die-casting-mold-material-selection-and-performance/
- https://www.asiatools.net/news/blog/how-to-select-mold-steel-for-die-casting-dies-h13-1-2344-thermal-fatigue-and-heat-checking-resistance
- https://firstmold.com/guides/heat-treatment/
- https://www.vacfurnace.com/vacuum-furnace-news/heat-treatment-process-of-die-casting-mold/
- https://gudmould.wordpress.com/2019/11/01/eight-technical-standards-of-die-casting-mold-that-must-be-observed/
- https://www.smithmetal.com/pdf/tool-steel/p20.pdf
- https://www.p20highhardsteel.com/page/the-hardness-of-p20-steel-varies-based-on-its-treatment-and-different-hardness-levels-30-34-hrc-34-38-hrc-39-44-hrc/67cebe7fdc5f3393f9a7966e
- https://www.hudsontoolsteel.com/technical-data/steelp0