The Short Answer: Start With 0.7 Percent, Then Adjust
For the common zinc die casting alloys, the usual starting point for mold design is a linear shrinkage allowance of about 0.7 percent. In decimal form that is 0.007 in/in or 0.007 mm/mm. In metric terms it is 7 mm per meter. In imperial terms it is approximately 0.084 in per foot. This is the conventional value used for Zamak 2, Zamak 3, Zamak 5, Zamak 7, and ZA-8, although individual alloy datasheets may list a narrow range around it, typically from about 0.006 to 0.0075 in/in depending on grade and supplier.
The important qualification is that 0.7 percent is a starting allowance, not a universal correction. Zinc die castings do not shrink uniformly in every direction. Freely shrinking sections may contract at roughly 0.6 to 0.8 percent, while sections restrained by cores, inserts, slides, or a rigid die wall may show an effective shrinkage of only 0.3 to 0.6 percent. Thin walls often freeze quickly and show lower shrinkage, while thick sections retain heat and tend to shrink more. Hotter dies and earlier ejection can leave more contraction to occur after the part leaves the mold. Zinc alloys can also undergo small dimensional changes after casting as they age.
A sound mold design therefore uses 0.7 percent as a baseline and then adjusts it feature by feature. For critical dimensions, the toolmaker should apply a conservative allowance, leave steel-safe stock, measure T1 samples, and make final corrections by grinding or EDM rather than by welding. The final allowance should always be confirmed with the die caster for the exact alloy, wall thickness, process window, and constraint condition.
Why Shrinkage Allowance Is a Mold Design Decision, Not a Material Constant
Shrinkage allowance is often described as a material property, but in die casting it is really a tooling decision. The mold cavity must be cut larger than the desired cold part dimension so that the casting can contract to its nominal size after solidification and cooling. If the cavity is cut exactly to the drawing, the finished part will usually be undersized. If the cavity is cut with an allowance that is too large, the part may be oversized, and the tool may need expensive correction.
The correct allowance depends on the interaction between the solidifying metal and the steel tool. A free external dimension can contract toward the center of mass with relatively little restraint. A bore formed by a core pin is different: the steel core physically occupies the space and restricts contraction while the casting is in the mold. The same is true for pockets, slots, and dimensions between inserts or slides. The result is that a single scale factor applied to the entire cavity can bring some features into tolerance while pushing others out.
Shrinkage allowance is also not a substitute for tolerance analysis. The nominal shrinkage correction moves the cavity from the nominal part size to an expected production size. It does not account for machine variation, die temperature variation, alloy batch variation, draft, machining stock, or post-cast aging. Those effects must be handled separately in the tolerance stack. A dimension that is critical at room temperature after weeks of aging needs a different treatment from a cosmetic feature that only needs to look correct after ejection.
The practical consequence is that mold design should begin with a clear classification of features. Which dimensions are free? Which are constrained by cores? Which are long, thin, or thick? Which will be machined after casting? Which must hold a tight tolerance over the life of the product? Once those questions are answered, the baseline shrinkage value can be adjusted intelligently rather than applied blindly.
Baseline Shrinkage Values for Common Zinc Alloys
The standard zinc die casting family is dominated by the Zamak alloys and the ZA alloys. Their shrinkage behavior is similar enough that a common baseline is useful, but different enough that the alloy should still be confirmed before steel is cut.
| Alloy | Typical linear shrinkage | Common mold design allowance | Notes |
|---|---|---|---|
| Zamak 3, ASTM AG40A | 0.6 to 0.7 percent | 0.006 to 0.007 in/in | Industry standard and usual default for dimensional stability |
| Zamak 5, ASTM AC41A | 0.6 to 0.7 percent | 0.006 to 0.007 in/in | Higher copper content raises strength; shrinkage similar to Zamak 3 |
| Zamak 2, ASTM AC43A | 0.6 to 0.7 percent | 0.006 to 0.007 in/in | Stronger alloy; may show small dimensional aging, so long-term tolerances need review |
| Zamak 7, ASTM AG40B | 0.6 to 0.7 percent | 0.006 to 0.007 in/in | High fluidity for thin walls; uses standard Zamak shrinkage practice |
| ZA-8 | 0.6 to 0.7 percent | 0.006 to 0.007 in/in | Hot-chamber castable zinc-aluminum alloy; close to standard Zamak behavior |
| ZA-12 and ZA-27 | 0.7 to 0.8 percent | 0.007 to 0.008 in/in | Higher aluminum content and cold-chamber casting usually require a slightly higher allowance |
For ordinary tooling in Zamak 3, many die casters and toolmakers use 0.007 in/in as the default. That is convenient because it is easy to remember and easy to apply in either metric or imperial units. It also sits near the upper half of the common range, which is often a sensible conservative choice for free-shrinking external dimensions. A 100 mm dimension becomes 100.7 mm in the cavity at 0.7 percent. A 250 mm dimension becomes 251.75 mm. A 12 in dimension becomes about 12.084 in.
However, the table should not be read as a guarantee. Some alloy suppliers publish a narrower range, such as 0.006 to 0.0075 in/in, and some foundry practice may favor a value closer to 0.006 for particular geometries. The alloy grade matters most when moving from standard Zamak to higher-aluminum ZA alloys, or when the part has unusually thick sections or long, constrained features. It is also important not to borrow shrinkage values from aluminum die casting. Aluminum alloys generally shrink more than zinc alloys, and applying an aluminum allowance to a zinc tool will produce oversized parts.
Free Versus Restricted Shrinkage
The most important adjustment to the baseline is the distinction between free and restricted shrinkage. A free feature is one that can contract without being held by a rigid part of the die. An outer perimeter, an isolated boss, or a dimension measured across a freely contracting mass may approach the full 0.6 to 0.8 percent range. A restricted feature is one where the steel core, insert, slide, or die wall prevents the casting from contracting as it cools. Internal bores, pockets formed around cores, and dimensions between rigid features often fall into this category.
In practical tooling, restricted dimensions may show an effective shrinkage of only about 0.3 to 0.5 percent, and some sources quote 0.3 to 0.6 percent depending on geometry and process. The exact value depends on how long the core remains in the part, how stiff the surrounding section is, how much draft and clearance are present, and how the part is ejected. A thin boss around a core may behave differently from a heavy section around the same core. A long core pin may restrain shrinkage along its length but allow more contraction at the free end.
The mistake to avoid is scaling the entire cavity by 0.7 percent and assuming every feature will land correctly. A better method is to scale the cavity for the general free-shrink behavior, then review constrained dimensions separately. For a critical bore, the designer should ask whether the core will be allowed to float, whether the part will shrink onto the core, and whether the final hole size will be controlled by the core diameter, by post-cast contraction, or by a subsequent machining operation. If the feature is truly constrained, forcing the full 0.7 percent allowance into the core dimension may produce a hole or pocket that is out of specification.
This is also where the concept of direction matters. Shrinkage is not a simple uniform reduction in all three axes. A long part may contract more along its length than across a stiff ribbed section. A boss may pull toward the main mass of the casting. A flat plate may warp if shrinkage is unbalanced. The mold designer should think in terms of constraint maps, not just a single percentage.
Wall Thickness and Thermal Gradients
Wall thickness changes the local cooling history, and cooling history changes shrinkage. Thin walls, typically below about 1.5 mm or 0.060 in, freeze quickly against the die surface. The metal may not have time to feed fully from the gate, and the section may show slightly lower effective shrinkage, often around 0.5 to 0.6 percent for free dimensions. Thick sections, typically above about 3.0 mm or 0.120 in, retain heat longer and can experience greater volumetric contraction, pushing the effective shrinkage toward 0.7 percent or more. Very thick sections may also suffer from sink, porosity, and internal shrinkage voids if gating and packing are not designed properly.
The best mold design practice is to keep wall thickness as uniform as the part function allows. Sudden transitions from thin to thick create thermal gradients, differential cooling, and uneven shrinkage. A thick boss attached to a thin wall can pull the wall during cooling, while a thin rib attached to a heavy section may freeze first and restrain the heavier section. These effects are not captured by a single shrinkage table. They require a review of the part geometry, gate location, cooling layout, and ejection strategy.
For mold design purposes, thick sections should generally be checked at the higher end of the free-shrink range, especially if the dimension is long and unconstrained. Thin sections can be checked at the lower end. But the designer should not overcorrect a thin wall to the point that the cavity is undersized. The final value should be confirmed by mold flow simulation where available and by T1 sample measurement in production.
Die Temperature, Ejection, and Process Effects
Shrinkage does not stop when the die opens. A part that is ejected at a higher temperature will continue to contract in air after ejection. Hotter die operating temperatures, shorter cooling times, and earlier ejection can therefore increase the apparent post-ejection shrinkage. A cooler die and a longer cooling time may reduce that effect, but they can also create flow marks, cold shuts, or poor surface finish if taken too far. The process window must be balanced.
Packing pressure and gate freeze also matter. If the gate freezes before the thick section has been packed, the section may shrink more than expected. If packing is maintained longer, the apparent shrinkage may be reduced. The die caster’s process settings are therefore part of the shrinkage equation. A tool that is dimensionally correct under one process window may drift when the process is optimized for cycle time or surface quality.
For critical dimensions, the mold designer should specify the expected die temperature range and ejection condition in the tool design review. The die caster should confirm whether the tool will be run hot or cold, whether the part will be air-cooled or water-cooled after ejection, and whether any fixture cooling will be used. These details can change the final size of long dimensions by a few hundredths of a millimeter, which may be enough to matter on a tight tolerance.
Alloy Chemistry and Post-Cast Dimensional Aging
Zinc alloys are not completely dimensionally inert after casting. Zamak 3 is generally valued for good dimensional stability and is often the default choice for parts that need consistent dimensions. Zamak 5 adds copper for strength and may show slightly more dimensional movement after casting. Zamak 2 is stronger still, but its aging behavior deserves attention when long-term tolerances are tight. The ZA alloys, with higher aluminum content, may also show different aging and shrinkage behavior, so the supplier’s specific data should be checked before cutting steel.
The direction of post-cast movement can be confusing because different sources describe aging as small growth or small shrinkage depending on alloy, section, and metallurgical condition. The practical point is not to memorize a single sign for every alloy. The practical point is that zinc castings can continue to change dimension after ejection, especially in the first weeks, with the rate diminishing over time. A part that is measured immediately after casting may not be the same size as a part that has been sitting in inventory for a month.
If a dimension must hold a tight tolerance over a long service life, the designer has two options. One is to include the expected aging movement in the tolerance stack and accept that the production window must be adjusted. The other is to specify a stabilizing heat treatment. Stabilization intentionally drives some of the dimensional change before the part is measured or machined. It typically produces a small additional shrinkage up front, on the order of 0.0004 to 0.0005 in/in in some practices, leaving less movement later. The exact treatment and allowance should be agreed with the die caster and the heat treater.
How to Calculate the Cavity Dimension
The basic calculation for a free-shrinking external dimension is straightforward:
Cavity dimension = part dimension × (1 + shrinkage allowance)
For a 100 mm part dimension and a 0.7 percent allowance, the cavity dimension is 100 × 1.007 = 100.7 mm. For a 250 mm dimension, it is 250 × 1.007 = 251.75 mm. For a 12 in dimension, it is 12 × 1.007 = 12.084 in. This is the same as adding 7 mm per meter or about 0.084 in per foot.
Some toolmakers prefer to divide by one minus the shrinkage instead of multiplying by one plus the shrinkage. The difference is small at zinc casting shrinkage levels, but the convention should be agreed at the start of the project so that the CAD model, the drawing, and the tool room use the same method. The important thing is consistency, not the exact algebraic form.
For constrained dimensions, the calculation should use a lower effective allowance. If a bore or pocket is expected to shrink at only 0.4 percent because of core restraint, the cavity or core dimension should be based on that lower value rather than the full 0.7 percent. The designer should also separate nominal shrinkage from tolerance. A shrinkage allowance moves the nominal tool size; it does not make the process capable of holding a tight tolerance. The tolerance stack should include mold machining tolerance, die wear, process variation, and post-cast aging.
A useful design review table might look like this:
| Design case | Suggested starting allowance | Action |
|---|---|---|
| General free zinc cavity scaling | 0.7 percent, or 0.007 in/in | Use as baseline for free external dimensions |
| Long unconstrained dimensions | Check at 0.6 to 0.8 percent | Review with die caster and simulation |
| Dimensions constrained by cores, inserts, or slides | Lower effective shrinkage, often 0.3 to 0.5 percent | Do not force the full 0.7 percent |
| Thin walls below about 1.5 mm | Often 0.5 to 0.6 percent for free dimensions | Check filling and packing |
| Thick sections above about 3.0 mm | Often near 0.7 percent or higher | Review sink, porosity, and packing |
| Tight, long-life dimensions | Baseline plus aging allowance | Consider stabilization and T1 validation |
A Practical Steel-Safe Tooling Strategy
For high-precision dimensions, the safest approach is to design the tool steel-safe. Steel-safe means leaving extra steel on cores or cavity walls so that the dimension can be adjusted later by grinding or EDM. If the trial sample shows that the feature is too small, the toolmaker can remove steel to enlarge the cavity or adjust the core. If the feature is too large, the correction is more difficult because welding can introduce stress, porosity, and surface finish problems. Welding is sometimes unavoidable, but it should not be the primary adjustment strategy on a new tool.
A practical steel-safe plan is to apply a conservative allowance of about 0.5 to 0.6 percent to critical features at the initial design stage, rather than the full 0.7 percent, and then leave stock on the steel. After T1 samples are measured, the toolmaker can make a precise correction. This is especially useful for bearing bores, center-to-center hole distances, mating bosses, and any dimension that is difficult to measure or correct after the tool is hardened.
The steel-safe strategy should be agreed with the die caster before the tool is cut. The die caster may have experience with the specific alloy and part family that suggests a different starting point. The tool designer should also document which features are steel-safe, how much stock is available, and what measurement method will be used on T1 samples. Without that documentation, the steel-safe allowance can be lost during machining or EDM.
A Step-by-Step Mold Design Workflow
A disciplined workflow reduces the risk of dimensional surprises. The following sequence is practical for most zinc die casting projects.
- Confirm the alloy. Identify whether the part will use Zamak 3, Zamak 5, Zamak 2, Zamak 7, ZA-8, ZA-12, or ZA-27. Obtain the supplier’s shrinkage data and aging recommendations.
- Classify the features. Separate free external dimensions, constrained bores and pockets, thin walls, thick sections, and dimensions that will be machined after casting.
- Apply the baseline. Use 0.7 percent, or 0.007 in/in, as the starting allowance for free zinc alloy dimensions. Use lower values for constrained features where appropriate.
- Review wall thickness. Adjust the allowance for thin or thick sections and check for thermal imbalance.
- Review the process window. Confirm die temperature, ejection temperature, cooling time, and packing pressure assumptions with the die caster.
- Check aging. For tight long-term tolerances, add an aging allowance or specify stabilization heat treatment.
- Design steel-safe. Leave stock on critical cores and cavity walls so that T1 corrections can be made by grinding or EDM.
- Validate with T1 samples. Measure the samples after a defined cooling and aging period, compare with the drawing, and correct the tool before production.
This workflow does not eliminate the need for experience, but it makes the assumptions visible. When a dimension goes out of tolerance, the team can trace whether the cause was alloy choice, constraint, wall thickness, process, aging, or tool correction.
Common Mistakes That Cause Dimensional Problems
The most common mistake is applying a single blanket shrinkage factor to the entire cavity. This is convenient in CAD, but it ignores constraint, wall thickness, and direction. A part can have some features that are perfect and others that are out of tolerance because the same percentage was used everywhere.
A second mistake is using the wrong alloy assumption. Zinc alloys are not aluminum alloys, and the ZA alloys are not identical to the Zamak alloys. A tool designed with an aluminum shrinkage value will usually produce zinc parts that are too large. A tool designed with a low zinc value for a high-aluminum ZA alloy may produce parts that are too small.
A third mistake is ignoring post-cast aging. If the part is measured immediately after ejection and the drawing tolerance is tight, the measurement may not represent the final size. The designer should define when the part will be measured and whether stabilization is required.
A fourth mistake is relying on welding to correct a tool that was cut too far from the target. Welding can be successful, but it is slower and less predictable than grinding or EDM from a steel-safe condition. A new tool should be designed so that the first correction is a steel removal operation.
A fifth mistake is treating shrinkage as a tolerance. Shrinkage allowance sets the nominal tool size. It does not guarantee that the process can hold a plus or minus tolerance. Process capability, die temperature control, and alloy consistency must be addressed separately.
FAQ
Is 0.7 percent always the correct shrinkage allowance for zinc die casting?
No. It is the conventional starting point for common zinc alloys such as Zamak 3, Zamak 5, Zamak 2, Zamak 7, and ZA-8, but the actual effective shrinkage depends on whether the feature is free or constrained, the wall thickness, the die temperature, the ejection condition, and post-cast aging. Use 0.7 percent as a baseline and adjust it for the specific feature.
Should I use a different allowance for holes and bosses?
Yes, in most cases. A boss that can shrink freely may approach the full 0.6 to 0.7 percent range. A hole or pocket formed around a rigid core may be restrained and may show only about 0.3 to 0.5 percent effective shrinkage. The mold designer should classify the feature and avoid applying the full free-shrink allowance to a constrained dimension.
How does wall thickness change the allowance?
Thin walls below about 1.5 mm often freeze quickly and may show lower free shrinkage, around 0.5 to 0.6 percent. Thick sections above about 3.0 mm retain heat longer and may shrink closer to 0.7 percent or more. Very thick sections also need a review of sink, porosity, and packing.
What about post-cast aging in zinc alloys?
Zinc die castings can continue to change dimension after ejection, especially in the first weeks. The direction and magnitude depend on the alloy and condition. For tight long-term tolerances, include aging in the tolerance stack or specify a stabilizing heat treatment. Stabilization drives some of the movement before final measurement and can reduce later dimensional drift.
When should I use a steel-safe design?
Use steel-safe design for critical dimensions such as bearing bores, center-to-center hole distances, mating bosses, and any feature that is difficult to correct after hardening. Apply a conservative initial allowance, leave extra steel on cores or cavity walls, measure T1 samples, and correct by grinding or EDM rather than welding.
Can mold flow simulation replace T1 sample measurement?
No. Simulation is valuable for predicting filling, cooling, and shrinkage trends, but it cannot fully capture alloy batch variation, machine behavior, die temperature distribution, and post-cast aging. Simulation should guide the initial design, while T1 samples and production measurements provide the final validation.
Conclusion
For zinc alloy die casting mold design, the most useful answer is a practical range rather than a single number. Start with about 0.7 percent linear shrinkage, equivalent to 0.007 in/in, 7 mm per meter, or 0.084 in per foot, for common zinc alloys such as Zamak 3, Zamak 5, Zamak 2, Zamak 7, and ZA-8. Treat 0.5 to 0.7 percent as the normal free-shrink working range, and reduce the effective allowance for dimensions constrained by cores, inserts, slides, or rigid die walls. Check thick sections at the higher end, thin sections at the lower end, and tight long-life dimensions against post-cast aging.
The best tooling strategy is conservative and adjustable. Apply the baseline, classify the features, design critical areas steel-safe, validate with T1 samples, and confirm the final allowance with the die caster. A mold designer who understands why shrinkage varies will make better decisions than one who simply applies a blanket percentage. The result is a tool that reaches dimensional approval faster, needs fewer weld repairs, and performs more consistently in production.
参考资料
- Zinc and aluminum die casting
- Search, page 53 – SAE International
- Casting Shrinkage of ZAC#1, ZAC#2 and Pure Zinc on Die Casting
- Casting Shrinkage of ZAC#1, ZAC#2 and Pure Zinc on Die Casting | CiNii Research
- Zinc Alloy Ingot
- How To Design Zinc Alloy Die Castings Effectively -DSW
- ODM Metal Die Casting: 7 Rules for Design Driven Parts
- Metal Casting Design Guide: Sand, Investment & Die Casting
- 5 Pattern Allowances in Casting: Shrinkage to Draft
- Design Guidelines for Zn Casting – ppt download